Koolfoam - EPS Physical Properties
Koolfoam EPS is manufactured in accordance with all elements of the Recognised Standard AS 1366 part 3 1992.
The numbers in the tables on this page represent minimum or maximum achieved values. Koolfoam EPS test results are available upon request.
All classes of Koolfoam EPS comply with AS2122.1
Density Chart - Grade of Koolfoam EPS Versus Weight pm3 (BP = Black Pearl)
| Unit | SL | S | H | VH | BP |
|---|---|---|---|---|---|
| Kg pm3 | 13 - 14 | 15 - 16 | 22 - 24 | 28 - 32 | 22 - 24 |
Compressive Stress at 10% Deformation (min)
| Unit | SL | S | H | VH | BP | Test |
|---|---|---|---|---|---|---|
| Kpa (min) | 70 | 85 | 135 | 165 | 135 | AS2498.3 |
Cross Breaking Strength (min)
| Unit | SL | S | H | VH | BP | Test |
|---|---|---|---|---|---|---|
| Kpa (min) | 135 | 165 | 260 | 320 | 135 | AS2498.4 |
Dimensional Stability (max) Length, Width and Thickness 70c Dry Condition, Seven Days (max)
| Unit | SL | S | H | VH | BP | Test |
|---|---|---|---|---|---|---|
| % (max) | 1 | 1 | 1 | 1 | 1 | AS2498.6 |
Flame Propagation Characteristics
| SL | S | H | VH | BP | Test | |
|---|---|---|---|---|---|---|
| Medium flame duration (max) s | 2 | 2 | 2 | 2 | 2 | AS2122.1 |
| Eighth value (max) s | 3 | 3 | 3 | 3 | 3 | |
| Medium volume retained % | 18 | 22 | 40 | 50 | 40 | |
| Eighth value (min) % | 15 | 19 | 37 | 47 | 37 |
AS 1530.3 -1999 Early Fire Hazard Properties
| Material | Ignitability Index (0-20) | Spread of Flame Index (0-10) | Heat Evolved Index (0-10) | Smoke Developed Index (0-10) |
|---|---|---|---|---|
| EPS | 12 | 0 | 3 | 5 |
BPIR
To simplify things for our customers, we provide the technical specifications of our products directly on our website. Should you require any additional information, feel free to ask.